PTFE INSIGHTS | Part 2 of 3
Explore the Series: Part 1 | Part 2 | Part 3
By Rodrigo Costa
Director of Engineering, Evantic
In our previous article, we introduced the amazing polymer Polytetrafluoroethylene (PTFE), highlighting its main properties, structure, and the types of PTFE resins commercially available. In this article, we will focus on the granular PTFE resins.
As mentioned in the previous article, granular resins are produced by the process known as Suspension Polymerization. This polymerization method includes little to no dispersing agent and high agitation at elevated temperature and pressure. The first reported polymerization of PTFE was by Dr. Roy Plunkett in 1941, and it was anything but commercial. The first reports of a process suitable for the manufacture of granular PTFE resins were reported in 1946. In simpler terms, polymerization of the TFE – which is a colorless and odorless gas – happens inside a reactor (also called a kettle or polykettle). The biggest challenge in the polymerization reaction is to remove the heat. That is the reason for vigorous agitation during the reaction and the use of water as a polymerization media. The agitation enhances the heat transfer to the cold water. If the heat is not controlled, it can result in overpressure and possible explosion of the reactor. The product of suspension polymerization is stringy-shaped particles (beads).
They are of variable size and shape and are elongated as a result of vigorous agitation, resembling shreds of grated coconut. Therefore, some finishing steps are required to give the polymer particles a more uniform particle size and allow for parts with usable properties to be manufactured. Figure 1 below shows the general steps involved in manufacturing granular PTFE resins.
The earlier article also touched on the homopolymer / copolymer designations. The normal convention of polymer science applies the name copolymer to any fluoropolymer resin containing more than 1% of a comonomer. If no comonomer is used in the polymerization process, the fluoropolymer is called virgin homopolymer. A fluoropolymer containing less than 1% comonomer is categorized as a modified homopolymer resin. That being said, most commercially available grades of granular PTFE resins are either virgin or modified homopolymers, following the definition of ASTM D4894. It is important to highlight that this ASTM standard does not cover mixtures of PTFE resin with additives such as colorants, fillers, or plasticizers, nor does it cover reprocessed or reground resin. Virgin and modified granular resins are further divided into two groups: low flow (or fine cut) and free flow (or pelletized). Due to the smaller molecular weight of the comonomer, the resultant molecular weight of a modified PTFE is smaller, however, the mechanical properties are improved, as well as the resistance to permeation. This occurs because the modifier reduces the crystal size within the polymer structure and reduces the melt viscosity. Therefore, during melting, particles flow better, improving void closure and consequently porosity, increasing specific gravity, among other properties.
Fine cut (low flow) resins have a typical average particle size in the range of 20 – 40 microns. The small particle size of fine cut PTFE resins imparts the highest physical properties possible to obtain from granular resins to the articles made with them. These powders have poor flow and relatively low apparent density (< 500 g/l). The small particle size of these resins renders them suitable for high quality skived films, big billets, and compounding with fillers such as glass fiber, carbon black, bronze, and others.
Pelletized (free flow) resins have a typical average particle size in the range of 450 – 550 microns and a bulk density above 500 g/l. Typically, mechanical and electrical properties of parts made with free-flow resins are lower than parts made with fine cut resins. However, processing can be more efficient as free-flow resins make it easier to fill molds and also require smaller molds.
As author Sina Ebnesajjad highlighted in his book Fluoroplastics – Volume 1: Non-Melt Processible Fluoroplastics, the Definitive User’s Guide and Databook [1], “It is important to note that, in spite of similarity of properties, no two resins are ever truly ‘equivalent’”. Often, manufacturers must make small but controlled changes to processing parameters in order to produce parts of similar properties when using different resins. OEMs can rely on Evantic’s knowledge and expertise to make parts with useful properties using the most suitable and economical resin.
Fabrication Methods
The most common way to produce parts from granular PTFE resins is by compression molding. In most cases, the molding process is employed to convert PTFE resins into basic, solid shapes: rods, cylinders, sheets, or blocks. Sizes can vary from diameters of a few inches up to more than 5 feet (more than 1.5 m) for rods and cylinders. Sheets can be as large as 48” x 48” (1.3 x 1.3 meters) and as thin as 0.063” (1.6 mm) up to 8” thick (203 mm).
In a compression molding process, PTFE powder is compressed inside a mold at ambient temperature. After removal from the mold, the preform is heated in an oven above its melting point and is sintered. Sintering is a heat treatment process, largely used in powder metallurgy and ceramics processing, for bonding particles into a coherent, solid structure via mass transport events that often occur on the atomic scale. The bonding leads to improved strength and lower system energy. In powder metallurgy and ceramics processing, the sintering temperature is slightly less than the material melting point. However, when sintering PTFE molded parts, the material temperature usually surpasses its melting point of 342°C. This is possible due to the exceptionally high melt viscosity of PTFE – the molten resin will not flow, having an appearance similar to a gelatin. Controlling the sintering temperature, among other molding and sintering parameters, enables manufacturers to control physical and mechanical properties of the parts produced.
The molded parts can further be machined in order to produce more complex parts such as manifolds, endcaps, valve seats, pump bodies, and more. Films can be produced by the process known as skiving – which consists of “peeling” layers of a desired thickness from a cylinder. Skived films (also referred to as sintered films) can be as thin as 0.001” (0.025 mm). Above 0.25” (6.35 mm) skived parts produced are called “sheets” and can be as thick as 0.375” (9.5 mm).
Main Properties
As a fully fluorinated polymer, PTFE is virtually inert to the most aggressive organic and inorganic chemicals and solvents over a wide temperature range. Chemical inertness means that PTFE can be in continuous contact with another substance with no detectable chemical reaction or degradation taking place.
Table 1 – PTFE properties relatively independent of processing conditions
| Chemical Properties | Electrical Properties | Mechanical Properties |
|---|---|---|
| Resistance to corrosive reagents | Low dielectric constant | Flexibility at low temperatures |
| Non-solubility | Low dissipation factor | Low coefficient of friction |
| Long-term weatherability | High arc resistivity | Stability at high temperatures |
| Non-adhesiveness | High surface resistivity | |
| Non-flammability | High volume resistivity |
Table 1 shows chemical, electrical, and mechanical properties relatively independent of processing conditions. In addition to the typical properties, modified granular PTFE grades offer weldability, improved resistance to deformation under load, increased permeation resistance, and higher dielectric breakdown voltage.
Literature has pointed out that about 15 mechanical properties plus several electrical and chemical properties are influenced by molding and sintering conditions such as compression pressure, dwell time under pressure, sintering temperature and time, and cooling rate. The most common properties influenced by these processing conditions are tensile strength and elongation, dielectric strength, permeability, flex life, resiliency, stiffness, and impact strength. There are five basic factors that influence these properties:
- Presence of Macroscopic Flaws: internal bubbles, tears, foreign impurities, shear planes, or poor charge-to-charge bonds
- Extent of Microporosity: number and size of microscopically visible voids created by imperfect particle fusion
- Percent of Crystallinity: a percentage based on the weight fraction of a sample consisting of polymer chains fitted in a close-packed, ordered arrangement
- Molecular Weight: a measure of the average length of polymer chains
- Degree of Orientation: a measure of the extent of alignment of polymer chains in a given direction
It’s not trivial to measure these characteristics directly, therefore indirect measurement methods have been devised: dielectric strength, tensile strength, ultimate elongation, specific gravity, and heat of fusion. Dielectric strength is a function of the degree of porosity, which can be evidenced by specific gravity and voids observation at 100x magnification; specific gravity, tensile strength, and elongation are functions of percent of crystallinity, molecular weight, and voids (microporosity and macroscopic flaws); tensile strength and elongation also indicate the degree of orientation. For example, an increase in the degree of crystallinity leads to an increase in elongation and specific gravity but decreases tensile strength and has almost no effect on dielectric strength. As a second example, higher molecular weight resins will produce parts with higher tensile strength, but elongation and specific gravity may be compromised while dielectric strength is minimally affected by molecular weight.
Common Applications for Parts Made of Granular PTFE Resin
- Chemical Processing Industry (CPI): In this industry, manufacturing is often carried out using highly corrosive fluids. PTFE’s chemical inertness and broad operating temperature range helps prevent corrosion and contamination, extending service life and preventing unscheduled downtime. Although sometimes more expensive initially, some PTFE components can minimize maintenance costs in the long run, helping companies to be more competitive. Evantic manufactures films, sheets, and custom machined parts such as manifolds, valve seats, diaphragms, and other complex parts that are used as components in CPI subsystems. If you have your own machining capabilities, we can supply the basic stock shapes to be turned into finished, machined parts.
- Piping: Flanged steel piping and a variety of fittings (T’s, elbows, reducers, spacers, etc.) are lined with PTFE tubes; also, PTFE is a standard material for gasketing due to its nearly universal chemical compatibility, good performance at temperatures from cryogenic to over 260°C, and conformability. PTFE is used alone, with fillers or metal supports, or as a dispersion for impregnating fibers such as aramids for gasketing. In addition to excellent sealing performance, gaskets made with PTFE can be used in a broad range of applications, so inventories can be reduced and there is less risk of misapplication.
- Sealing: The almost universal chemical compatibility and the broad operating temperature already mentioned, allied to the low coefficient of friction, make PTFE a great material for sealing purposes. PTFE is largely used either as an entirely made seal or as a component. In seats and packings, it provides conformability – that is, the parts conform to mating surfaces for good sealing – and low friction for ease of operation. For diaphragms, PTFE provides good flex life. Seals for rotating or sliding shafts use elements of PTFE compounded with fillers such as graphite. PTFE is used alone, with fillers or metal supports, or as a dispersion for impregnating fibers such as aramids for gasketing.
- Semiconductor Processing: In semiconductor manufacturing, wet processing equipment, fluid transport systems, and wafer handling have relied on PTFE parts since these processes are extremely intolerant of particulate and chemical contamination that, even in trace amounts, can cause a severe decrease in yields. PTFE’s resistance to chemical attack, combined with Evantic’s capability to manufacture high purity basic shapes and machined parts, is therefore, an important attribute for this application.
- Bearings: Due to its inherent low friction and lubricity, PTFE is often used in bearings and bushings. It can be compounded with other materials such as bronze, graphite, and other special fillers to reduce creep and improve wear resistance and/or thermal conductivity, for example. In this application, PTFE is usually applied to a metal support (substrate). In order for PTFE to bond, it must be chemically etched. Evantic offers chemically etched PTFE parts enabling the parts to be bonded to metal and other substrates.
If you are looking for a basic molded PTFE shape, a more complex geometry (machined part), or any kind of PTFE films or sheets, don’t hesitate to contact us. Our team of specialists will be happy to assist you with material selection and defining the properties needed to supply the parts that are right for your application.
Check our website www.evantic.com for more information or contact us at sales@evantic.com.
REFERENCES
[1] Ebnesajjad, Sina. Fluoroplastics – Volume 1: Non-Melt Processible Fluoroplastics, the Definitive User’s Guide and Databook. 2nd ed., Elsevier, 2015.
[2] Sperati, C. A., and H. W. Starkweather. “Fluorine-Containing Polymers. II. Polytetrafluoroethylene.” Fortschritte Der Hochpolymeren-Forschung Advances in Polymer Science, 1961, 465–95.
[3] Teflon PTFE: Compression Molding. Teflon PTFE: Compression Molding, The Chemours Company, 2019
[4] DuPont. DuPont Fluoropolymers: An Introduction to DuPont Fluoropolymers. DuPont Fluoropolymers: An Introduction to DuPont Fluoropolymers, DuPont, 2012.